Page 44 - 《摩擦学学报》2020年第5期
P. 44

第 5 期                 李平, 等: 回火温度对20Cr13不锈钢液固两相流冲刷腐蚀性能的影响                                    599

            严重. 650 ℃回火的20Cr13不锈钢的组织中出现较大                          steel  at  different  locations  of  a  90°  elbow[J].  Corrosion  Science,
            颗粒的碳化物,导致基体中Cr分布不均匀,耐腐蚀性                               2016, 111: 72–83. doi: 10.1016/j.corsci.2016.05.004.
                                                               [  7  ]  Dong C F, Xiao K, Li X G, et al. Erosion accelerated corrosion of a
            变差,又因为基体组织为索氏体,硬度较低,抗冲刷磨
                                                                   carbon steel–stainless steel galvanic couple in a chloride solution[J].
            损能力较弱,因而在料浆液和固体颗粒的冲刷腐蚀联
                                                                   Wear, 2010, 270(1-2): 39–45. doi: 10.1016/j.wear.2010.09.004.
            合作用下,试样表面出现了严重的腐蚀坑和剥落.
                                                               [  8  ]  Robert J K Wood. Erosion–corrosion interactions and their effect on
            3    结论                                                marine and offshore materials[J]. Wear, 2006, 261(9): 1012–1023.
                                                                   doi: 10.1016/j.wear.2006.03.033.
                a. 20Cr13不锈钢经过1 030 ℃油淬,在250~700 ℃             [  9  ]  Huang  Weijiu,  He  Haoran,  Wang  Zhenguo,  et  al.  Cavitation  and
            回火,组织由马氏体转变为屈氏体、索氏体,钢中碳化                               erosion behavior of tin brass in multiphase flow[J]. Tribology, 2018,
                                                                   38(4): 410–416 (in Chinese) [黄伟九, 何浩然, 王振国, 等. 多相流
            物颗粒变大;250 ℃硬度最高,随回火温度升高,硬度
                                                                   作用下锡黄铜的空蚀-冲蚀行为[J]. 摩擦学学报, 2018, 38(4):
            先稍微降低,回火温度高于500 ℃以后硬度快速下降.
                                                                   410–416]. doi: 10.16078/j.tribology.2018.04.005.
                b. 随回火温度升高,20Cr13不锈钢的自腐蚀电流
                                                               [10]  Li  Guangyu,  Qi  Senpeng,  Yu  Kewei,  et  al.  Wear  and  corrosion
            密度逐渐增大,250 ℃回火处理试样的耐腐蚀性能最                              resistance  of  plasma  source  nitrided  2Cr13  martensitic  stainless
            好;不同回火温度20Cr13不锈钢在0.5M H SO +10%                       steel[J]. Materials for Mechanical Engineering, 2019, 43(4): 6–9, 34
                                                 2
                                                     4
            石英砂料浆中的冲刷腐蚀特征表现为腐蚀作用强于                                 (in Chinese) [李广宇, 齐森鹏, 于克伟, 等. 等离子体源渗氮
            冲刷作用,而冲刷强烈促进腐蚀,冲刷与腐蚀的交互                                2Cr13马氏体不锈钢的耐磨与耐腐蚀性能[J]. 机械工程材料,
                                                                   2019, 43(4): 6–9, 34]. doi: 10.11973/jxgccl201904002.
            作用量占总冲刷腐蚀量的80%左右.
                                                               [11]  Liu  Zhengwu,  Zhu  Xiaogang,  Sun  Jing,  et  al.  Microstructure  and
                c. 20Cr13不锈钢冲刷腐蚀后表面呈现出挤压锻
                                                                   mechanical properties of 2Cr13 stainless steel using selective laser
            打和犁削作用造成的凹坑和沟痕,250 ℃回火时试样
                                                                   melting[J]. Applied Laser, 2019, 39(3): 411–415 (in Chinese) [刘正
            冲刷腐蚀量最低,耐冲刷腐蚀性最好,表明采用适当                                武, 朱小刚, 孙靖, 等. 激光选区熔化成形2Cr13不锈钢组织与力学
            的回火温度可以显著改善20Cr13不锈钢的抗冲刷腐                              性能研究[J]. 应用激光, 2019, 39(3): 411–415].
            蚀磨损性能.                                             [12]  Shao  Tianmin,  Hua  Meng,  Tam  Hon  Yuen,  et  al.  Impact  wear
                                                                   behavior of laser hardened hypoeutectoid 2Cr13 martensite stainless
            参 考 文 献
                                                                   steel[J]. Wear, 2003, 255(1-6): 444–455. doi: 10.1016/S0043-1648
            [  1  ]  Wang Linqing, Zhou Yongtao, Wang Junjun, et al. Corrosion-wear  (03)00417-4.
                 interaction behavior of TC4 titanium alloy in simulated seawater[J].  [13]  Wang  Pinghuai,  Wang  Bojian,  Song  Jingna,  et  al.  Influence  of
                 Tribology, 2019, 39(2): 206–212 (in Chinese) [王林青, 周永涛, 王  quenching temperature on microstructure and performance of 2Cr13
                 军军, 等. TC4钛合金在模拟海水中腐蚀-磨损交互行为研究[J].                stainless  steel[J].  Hot  Working  Technology,  2008,  37(4):  71–73
                 摩 擦 学 学 报 ,  2019,  39(2):  206–212].  doi:  10.16078/j.tribology.  (in Chinese) [王平怀, 王伯健, 宋景娜. 淬火温度对2Cr13不锈钢组
                 2018086.                                          织和性能的影响[J]. 热加工工艺, 2008, 37(4): 71–73]. doi: 10.3969/
            [  2  ]  Adnan, A N, K im, M H. Erosion wear on centrifugal pump casing  j.issn.1001-3814.2008.04.023.
                 due to slurry flow[J]. Wear, 2016, 364-365: 103–111. doi: 10.1016/  [14]  Yan Yinxia, Zhao Hongmin, Gong Xinyong, et al. Heat treatment of
                 j.wear.2016.07.005.                               2Cr13  stainless  steel  valve  body[J].  Heat  Treatment,  2013,  28(6):
            [  3  ]  Li P, Cai Q Z, Wei B K, et al. Failure analysis of the impeller of  35–38 (in Chinese) [严银霞, 赵洪敏, 宫心勇, 等. 2Cr13不锈钢阀
                 slurry  pump  used  in  zinc  hydrometallurgy  process[J].  Engineering  体的热处理[J]. 热处理, 2013, 28(6): 35–38]. doi: 10.3969/j.issn.
                 Failure Analysis, 2005, 13(6): 876–885.           1008-1690.2013.06.011.
            [  4  ]  Rahul  Tarodiya,  Bhupendra  K  Gandhi.  Experimental  investigation  [15]  Zhu  Xiangqun,  Dai  Qixun,  Zhou  Ming,  et  al.  Effect  of  tempering
                 of  centrifugal  slurry  pump  casing  wear  handling  solid-liquid  temperature on stress-corrosion cracking and mechanical hysteresis
                 mixtures[J]. Wear, 2019, 434-435(15): 1–11.       of  2Cr13  stainless  steel[J].  Transactions  of  Materials  and  Heat
            [  5  ]  Jin  Haozhe,  Yi  Yuwei,  Liu  Xu,  et  al.  Simulation  and  analysis  of  Treatment, 2009, 30(1): 11–14, 19 (in Chinese) [朱向群, 戴起勋, 周
                 erosion characteristics in flushing oil pipeline with liquid-solid phase  明, 等. 回火温度对2Cr13不锈钢应力腐蚀开裂和力学滞后的影响
                 fluids[J]. Tribology, 2016, 36(6): 695–702 (in Chinese) [金浩哲, 易  [J]. 材料热处理学报, 2009, 30(1): 11–14, 19].
                 玉微, 刘旭, 等. 液固两相流冲洗油管道的冲蚀磨损特性数值模拟              [16]  Liu Yurong, Ye Dong, Yong Qilong, et al. Effect of heat treatment
                 及 分 析 [J].  摩 擦 学 学 报 ,  2016,  36(6):  695–702].  doi:  10.16078/  on microstructure and property of Cr13 super martensitic stainless
                 j.tribology.2016.06.005.                          steel[J].  Journal  of  Iron  and  Steel  Research,  International,  2011,
            [  6  ]  Zeng  L,  Shuang  S,  Guo  X  P,  et  al.  Erosion-corrosion  of  stainless  18(11): 60–66. doi: 10.1016/S1006-706X(11)60118-0.
   39   40   41   42   43   44   45   46   47   48   49